Research Institutions: Institute of Plasma Physics, Chinese Academy of Sciences & Shanghai University of Engineering Science
Abstract
This research proposes and systematically verifies a pre-filled narrow-gap laser oscillation welding technology, providing a comprehensive analysis of how laser oscillation remodels the thermodynamic and fluid dynamics behavior inside ultra-deep molten pools. The findings address a critical industry challenge: the persistent problem of sidewall lack of fusion in thick plate welding, which has long plagued nuclear power, aerospace, and heavy equipment manufacturing sectors.
Key Findings
- Energy Distribution Optimization
Oscillation technology fundamentally breaks the traditional highly concentrated single-peak energy distribution characteristic of laser welding. This innovation significantly reduces the peak energy density from 1067 J/mm² to 772.9 J/mm², effectively preventing excessive heat input at the weld center while greatly improving local heat accumulation at the sidewall boundary.
- Flow Pattern Transformation
When oscillation parameters are optimized to 1.8 mm amplitude and 40 Hz frequency, the laser's lateral heating area is effectively expanded, causing the molten pool size to transform from "narrow and long" to "wide and shallow" (increased width, shortened length). The strong mechanical stirring effect generated by these parameters successfully overcomes flow limitations dominated by surface tension.
The disordered, easily skewed asymmetric flow pattern typical of non-oscillating laser welding is forcibly converted into an ordered, symmetric strong convection mode, accelerating the radial scouring and transport of high-temperature liquid metal to both sidewalls.
- Mathematical Process Window Derivation
The study rigorously derives and verifies a mathematical process window for defect suppression: ``` 1 ≤ 2A/D ≤ 1.5 ``` Where A = oscillation amplitude, D = gap width. This window grants the welding process extremely high anti-interference capability. Within this interval, process stability is significantly enhanced.
- Full Cycle Dynamic Behavior
The research deeply reveals the decisive regulatory effect of oscillation amplitude on the dynamic evolution of molten pool cross-sectional morphology within a complete oscillation cycle:
- Small amplitude: Highly concentrated laser energy results in a narrow-bottom conical molten pool, with sidewalls heated only by limited heat conduction, leading to unilateral inclination and lack of fusion defects.
- Increased amplitude: Heat dynamically accumulates at the interface between the preset plate and sidewalls, gradually broadening the molten pool bottom into a U-shape.
- Optimized large amplitude: Laser energy achieves uniform lateral redistribution, significantly enhancing sidewall wetting characteristics and penetration depth. Within a complete left-right oscillation cycle, the molten pool overcomes thermal hysteresis effects and continuously accumulates heat under the combined action of direct irradiation and heat conduction, expanding alternately to both sides as the beam moves, ultimately establishing a perfectly symmetrical central morphology.
Performance Improvements
- Defect elimination: Sidewall lack of fusion defects are completely eliminated within the optimized parameter range
- Stability: High-frequency disturbance significantly improves the overall stability of the keyhole and molten pool
- Wetting conditions: Sidewall wetting conditions are markedly improved, ensuring effective fusion between the weld and sidewalls
- Quality consistency: Weld quality consistency is dramatically enhanced, reducing post-weld inspection and rework requirements
Industrial Significance
This technology provides a reliable solution for high-quality welding of thick plates in nuclear power equipment, pressure vessels, and large structural components. The validated process window offers clear guidance for industrial application, enabling manufacturers to achieve consistent, high-quality welds with reduced reliance on highly skilled manual welders. The findings represent a significant advancement in thick plate laser welding technology, with immediate applicability to the manufacturing of critical infrastructure components.