Research Team and Funding
A joint research team from CRRC Qingdao Sifang Rolling Stock Co., Ltd., the State Key Laboratory of Precision Welding and Joining of Materials and Structures at Harbin Institute of Technology, the Shandong Provincial Key Laboratory of Special Welding Technology at Harbin Institute of Technology (Weihai), and the Shandong Shipbuilding Technology Research Institute has published new findings on laser-TIG hybrid welding of a new generation of high-strength Al-Mg-Zn aluminum alloy. The work was supported by the National Key R&D Program of China (grant 2023YFB3710400) and appeared in the July 2026 issue of Electric Welding Machine (DOI: 10.7512/j.issn.1001-2303.2026.07.02). The first author, Dr. Liu Fuyun, is an assistant researcher whose work focuses on laser welding of light alloys and intelligent welding.
Why It Matters
The new Al-Mg-Zn alloy is a core candidate material for lightweight rail transit car bodies, where reducing structural weight directly translates into energy savings and higher payload. However, fusion welding of this alloy has long been hampered by two stubborn problems: porosity in the weld metal and softening (strength loss) in the heat-affected zone. The team set out to map how laser power controls these defects and to identify a process window that produces sound, mechanically reliable joints.
Experimental Setup
The researchers carried out laser-TIG hybrid welding on 4 mm thick T6-tempered Al-7Mg-3Zn plate. Three laser power levels — 2.0, 2.4, and 2.8 kW — were compared, while other process variables were held constant. The resulting welds were characterized by metallographic observation, ImageJ-based image analysis of pore area, microhardness mapping, and room-temperature tensile testing. Combining the deep-penetration keyhole of a laser with the stable arc and filler-metal tolerance of TIG is a well-established strategy for aluminum, but the interaction between the two heat sources makes porosity behavior highly sensitive to parameter choice.
Key Findings
Practical Implications
For rail-transit manufacturers evaluating Al-Mg-Zn carbody structures, the study provides a concrete process-window lesson: simply turning up laser power to gain penetration is counterproductive because it re-introduces keyhole porosity in Mg- and Zn-bearing alloys. A moderate laser setting paired with TIG arc stabilization delivers the best balance of penetration, pore control, and mechanical properties. The results also support the broader trend in Chinese welding research toward physics-informed parameter selection — using measurements of pool dynamics, evaporation behavior, and solidification time rather than empirical trial-and-error — which is increasingly being paired with in-process sensing and closed-loop control on production lines.
Publication Details
- Journal: Electric Welding Machine, 2026, 56(7): 10–16
- DOI: 10.7512/j.issn.1001-2303.2026.07.02
- Received: 2025-12-26; Revised: 2026-01-19; Print publication: 2026-07-20
- Authors: Liu Fuyun, Qi Weining, Zhou Xiaohui, Lin Danyang, Tan Caiwang, Han Xiaohui, Song Xiaoguo, et al.